Forging and Casting
Open in the Padhaiko app6.1 Introduction, forging tools, forging operations
Forging is a metal-forming process in which solid metal is shaped by localized compressive forces—applied through manual hammer blows, power hammers, or presses—typically after heating the metal to its plastic (forging) temperature range.
- Forging Temperature Range: Mild steel (low-carbon steel) is forged between 850 deg C and 1250 deg C (cherry red to bright yellow heat). Overheating until white sparks fly ("burning") permanently ruins grain boundaries; hammering below ~800 deg C risks work-hardening and cracking.
- Advantages of Forging: Compresses internal porosity, refines coarse grains into fine grains, and aligns metal grain flow lines smoothly around corners and fillets—making forged crankshafts, connecting rods, spanners, and hooks much stronger and tougher than cast or machined equivalents.
- Smith (Open-Die) vs. Drop (Closed-Die) Forging: Hand/smith forging shapes heated stock freely between flat or simple shaped dies on an anvil; closed-die forging forces hot billet metal into precision die cavities for mass production.
Forging Tools
| Category | Tool Name | Construction & Primary Function |
|---|---|---|
| Heating | Smith's Forge (Hearth) | Brick/cast-iron hearth burning coke/coal with a bottom air tuyere, centrifugal blower, exhaust hood, and water slack tank |
| Supporting | Anvil | Heavy steel-faced cast block featuring a flat hardened face, tapered horn (beak) for bending curves, step for cutting, square hardy hole (holds hardie/swage shanks), and round pritchel hole (for punching) |
| Supporting | Swage Block | Heavy perforated cast-iron block with semicircular, V, and square edge grooves plus square/round through holes for bending and sizing |
| Holding | Tongs | Long-handled hinged gripping tools: flat-bit tongs (flat stock), hollow/round-bit tongs (round bars), pick-up tongs, and box/link tongs |
| Striking | Ball-Peen, Cross-Peen & Sledgehammers | Smith guides work with 1–2 kg hand hammer; helper strikes heavy blows with 4–8 kg sledgehammer |
| Shaping | Fullers (Top & Bottom) | Rounded necking tools used in pairs to groove stock and draw down metal rapidly without sharp stress notches |
| Shaping | Swages (Top & Bottom) | Semicircular grooved dies used in pairs to finish round, hexagonal, or octagonal bars smooth and concentric |
| Smoothing | Flatter & Set Hammer | Broad flat-faced flatter smooths hammer marks on flat surfaces; small set hammer forms crisp square corners and shoulders |
| Cutting & Piercing | Hot Set, Cold Set, Hardie, Punch & Drift | Hardie fits anvil hardy hole to cut hot bars from below; hot chisel (set) cuts hot stock; punch & tapered drift pierce and size holes |
Forging Operations
- Upsetting (Jumping): Increasing the cross-sectional area of a heated section at the expense of its length by hammering axially along the bar (for example, forming bolt heads or collars). Heat only the local portion to be upset so the rest stays rigid.
- Drawing Down (Drawing Out): Increasing the length of a bar while reducing its thickness/cross-section, using a cross-peen hammer or top-and-bottom fullers, then smoothing with a flatter or swage.
- Bending: Forming right-angle corners (over the sharp anvil edge, supported to avoid necking) or smooth rings and eyes (around the conical anvil horn).
- Punching and Drifting: Driving a hot punch halfway through from one side, flipping the job over to punch through cleanly from the back (preventing a ragged burr) over the pritchel/hardy hole, and sizing with a tapered drift.
- Cutting Off: Nicking and shearing hot stock over the hardie edge or with a long-handled hot chisel (never hammer all the way onto the bare hard steel anvil face; finish the final cut over a soft iron cutting plate or the step).
- Forge Welding: Heating two low-carbon steel / wrought-iron ends to white welding heat (~1300 deg C), sprinkling borax flux to dissolve surface scale, and hammering rapidly together to fuse in the solid plastic state.
Volume Conservation in Forging
Plastic forging deforms metal without adding or removing mass (ignoring tiny scale loss). Therefore, initial heated volume equals final forged volume: V_initial = V_final ==> A1 x L1 = A2 x L2
- For a cylindrical bar of diameter d and heated length L: (pi / 4) x d1^2 x L1 = (pi / 4) x d2^2 x L2
- For a rectangular/square bar of cross-section A1 and length L1: A1 x L1 = A2 x L2
6.2 Introduction, pattern making foundry tools, core making, sand casting process
Casting (Foundry Practice) is a manufacturing process in which molten metal is poured into a refractory mould cavity of the desired geometry and allowed to solidify and cool into a solid component. Casting excels at producing complex internal passages, hollow engine blocks, pump housings, and massive machine frames in a single piece.
Pattern Making and Allowances
A pattern is a full-scale replica of the object to be cast, made from seasoned wood (teak, pine, mahogany), cast aluminium, brass, or epoxy plastic, modified with dimensional allowances and core prints.
- Common Pattern Types:
- Single-piece (Solid) pattern: One-piece pattern for simple flat shapes.
- Split (Two-piece) pattern: Divided along the parting plane and aligned with dowel pins; top half goes in the cope, bottom half in the drag.
- Loose-piece pattern: Removable projections withdrawn separately sideways after the main pattern is lifted.
- Match-plate & Gated patterns: Multiple patterns mounted permanently on a plate or joined by runner/gate bars for high-volume moulding.
Four Essential Pattern Allowances
- Shrinkage (Contraction) Allowance: Added to all linear dimensions to compensate for solid thermal contraction as the solidified metal cools down to room temperature (applied directly with a contraction scale / shrink rule). Typical values:
- Grey Cast Iron: ~10 mm/m (1%)
- Brass / Copper / Aluminium: ~13 to 16 mm/m (1.3–1.6%)
- Carbon Steel: ~20 mm/m (2%)
- Draft (Taper) Allowance: Slight vertical taper (1 to 3 degrees on external walls, slightly more on internal pockets) enabling the pattern to be drawn cleanly out of the rammed sand without tearing mould walls.
- Machining (Finishing) Allowance: Extra stock (1.5 to 5 mm per face, larger on cope/top surfaces where slag floats) added on surfaces that will later be turned, bored, or milled smooth.
- Distortion (Camber) & Shake Allowances: Opposite pre-camber bent into U- or T-shaped patterns to counter uneven cooling warpage; shake (rapping) allowance is a slight negative allowance offsetting cavity enlargement when a pattern is rapped loose.
Foundry Tools and Moulding Sand
- Moulding Sand Composition: Standard green sand consists of silica sand (75–85%) for refractoriness, clay/bentonite binder (8–15%) for green strength, water (4–6%) to temper the clay, and additives like sea-coal dust (2–5%, improves surface finish on iron castings) or wood flour. (Green sand is used moist without baking; dry sand moulds are oven-baked for large heavy castings.)
| Tool | Description & Function |
|---|---|
| Moulding Flasks (Boxes) | Rigid rectangular wooden/metal frames holding rammed sand: Drag (bottom box), Cope (top box), and Cheek (intermediate box for 3-part moulds) |
| Riddle & Shovel | Wire-mesh sieve (riddle) screens fine facing sand onto the pattern face; shovel mixes and loads backing sand |
| Rammers (Peen & Butt) | Peen rammer (wedge end) packs sand tight in corners and flask edges; butt rammer (flat end) compacts flat sand layers evenly |
| Strike-Off Bar | Straight metal/wood bar scraped across the flask rim to level excess rammed sand flush |
| Vent Wire | Thin stiff steel needle pierced repeatedly through sand almost to the pattern so steam and mould gases escape during pouring |
| Trowel, Slick & Lifter | Flat trowel smooths parting faces; spoon-ended slick repairs broken corners; L-shaped lifter scoops loose sand from deep pockets |
| Sprue Pin & Riser Pin | Tapered wooden pins rammed inside the cope to leave vertical channels: sprue (molten metal entry) and riser (shrinkage-feeding reservoir & gas indicator) |
| Gate Cutter & Swab | U-shaped gate cutter carves horizontal runner/ingate channels connecting the sprue base to the mould cavity; swab moistens sand edges before pattern draw |
| Draw Spike & Bellows | Pointed steel spike driven into the pattern to rap and lift it cleanly; bellows blow loose sand particles out of the cavity |
Core Making
A core is a pre-formed, hardened sand body placed inside the mould cavity to produce internal holes, hollow chambers, or undercuts that cannot be formed directly by the pattern.
- Core Prints: Matching projections attached to the pattern that create recessed seats in the sand mould to locate and hold the core ends securely against buoyant molten metal lift.
- Core Making Steps:
- Mix clean clay-free silica sand with an organic/chemical binder (core oil, dextrin, molasses, or sodium silicate / resin).
- Pack the core sand firmly into a split core box, insert reinforcing core wires/arbors if slender, and pierce vent holes through the core axis.
- Turn the green core out onto a flat metal core plate and bake it in a core oven (180–250 deg C) until hard and permeable.
- Trim parting fins, join split core halves with core paste, coat with refractory graphite/zircon wash, and seat snugly into the mould's core prints (adding thin sheet-metal chaplets between mould and core if an overhang needs extra support).
Sand Casting Process (Step-by-Step)
- Pattern & Core Selection: Prepare the pattern with allowances and bake the required cores.
- Drag Moulding: Place the bottom pattern half on a flat moulding board inside the drag (inverted), dust parting sand (dry silica/lycopodium) so sand won't stick, riddle a 25 mm layer of fine facing sand over the pattern, fill with backing sand, ram with peen and butt rammers, strike off flush, vent, and roll the drag upright.
- Cope Moulding: Place the top pattern half onto the drag using dowel pins, dust dry parting sand across the parting line, clamp the cope box on top, position the tapered sprue pin and riser pin, riddle facing sand, fill, ram, strike off, and pierce vent holes.
- Pattern Withdrawal & Gating: Pull out the sprue and riser pins (carving a funnel-shaped pouring basin at the sprue top). Lift the cope carefully and set it aside. Lightly moisten pattern edges with a swab, tap gently with a draw spike (rapping), lift the pattern halves cleanly, carve horizontal runner and ingates in the drag with a gate cutter, repair any damaged edges with slicks, and blow out loose sand.
- Core Setting & Mould Closing: Seat the baked core firmly into the core prints, lower the cope smoothly back onto the drag aligned by guide pins, and clamp/weight down the cope so molten metal buoyancy cannot float it up.
- Melting & Pouring: Melt the charge (cast iron in a cupola, aluminium/brass in a crucible furnace) and pour smoothly in a steady stream down the pouring basin until molten metal rises in the riser.
- Shakeout, Fettling & Inspection: After solidification and cooling, break open the sand mould (shakeout), cut off gates/sprues/risers and grind flash fins (fettling), knock out core sand, and inspect for defects (blowholes, shrinkage cavities, cold shuts, misruns).
Worked Examples
1
A grey cast iron flanged collar has finished machined dimensions:
- Outside diameter = 200 mm
- Central bore diameter = 80 mm
- Axial length = 60 mm
All external, bore, and end faces require a 2.5 mm machining allowance per surface, and the shrinkage allowance for grey cast iron is 10 mm/m (1%). Calculate the exact wooden pattern and core-box dimensions (outside diameter, bore diameter, and length).
Determine rough casting dimensions (applying machining allowance):
- Rough cast outside diameter = 200 + (2 x 2.5) = 205.0 mm
- Rough cast bore diameter = 80 - (2 x 2.5) = 75.0 mm
- Rough cast length = 60 + (2 x 2.5) = 65.0 mm
Apply 1% grey cast-iron shrinkage allowance (10 mm/m = 0.01) to obtain pattern/core-box sizes: Because the solid ring contracts radially upon cooling (both OD and ID shrink), multiplying rough cast dimensions by (1 + 0.01) = 1.01 gives the physical pattern and core-box sizes:
- Pattern outside diameter: 205.0 x 1.01 = 207.05 mm (approx. 207.1 mm)
- Core-box bore diameter: 75.0 x 1.01 = 75.75 mm (approx. 75.8 mm)
- Pattern length: 65.0 x 1.01 = 65.65 mm (approx. 65.7 mm)
Pattern OD = 207.05 mm, core-box bore ID = 75.75 mm, pattern length = 65.65 mm.
2
Using volume conservation during hot forging (neglecting scale loss): (a) A 20 mm diameter mild steel round bar is heated over a 60 mm end length and upset uniformly to form a 30 mm diameter cylindrical head. Find the new forged length of the head. (b) A 30 mm x 30 mm square steel bar of length 100 mm is drawn down to a 20 mm x 20 mm square bar. Find its new length.
(a) Upsetting a 20 mm round bar to 30 mm diameter:
- Equate cylindrical volumes: (pi / 4) x d1^2 x L1 = (pi / 4) x d2^2 x L2
- L2 = L1 x (d1 / d2)^2 = 60 x (20 / 30)^2 = 60 x (4 / 9) = 240 / 9 = 26.67 mm.
(b) Drawing down a 30 mm square bar to 20 mm square:
- Initial volume V1 = 30 x 30 x 100 = 90000 cu mm.
- Final cross-sectional area A2 = 20 x 20 = 400 sq mm.
- Final length L2 = V1 / A2 = 90000 / 400 = 225.0 mm.
(a) Upset head length = 26.67 mm; (b) Drawn-down length = 225.0 mm.
3
Describe the step-by-step green-sand moulding procedure to cast a hollow cylindrical sleeve using a split (two-piece) pattern with core prints and a baked cylindrical sand core.
Prepare the drag half of the mould:
- Place the bottom half of the split pattern (with core-print projections at both ends) flat-face down on a clean moulding board, and set the inverted drag flask around it.
- Dust dry parting sand lightly over the pattern, riddle a 25 mm layer of fine facing sand over it, fill with tempered green backing sand, and ram evenly with peen (around edges) and butt rammers.
- Scrape excess sand flush with a strike-off bar, prick gas vent holes with a vent wire, place a bottom board on top, and roll the drag upright.
Prepare the cope half, withdraw pattern, and set the core:
- Smooth the parting surface, align the top pattern half onto the bottom half using dowel pins, dust parting sand, and place the cope box on top.
- Stand tapered sprue and riser pins vertically beside the pattern, riddle facing sand, fill, ram, strike off, and vent the cope.
- Pull out the sprue and riser pins, carve a pouring basin, lift off the cope carefully, swab edges lightly, rap and lift both pattern halves using a draw spike, and cut horizontal runner and ingates in the drag with a gate cutter.
- Blow loose sand out with bellows, seat the baked cylindrical sand core horizontally into the left and right core prints, close and clamp the cope onto the drag, and pour molten metal smoothly until it fills the riser.
Ram the drag around the bottom split pattern -> roll over -> align top pattern half, sprue, and riser pins -> ram the cope -> remove pins, separate cope, draw pattern halves, and cut runner/gates -> seat the baked sand core into core prints -> close, clamp, and pour molten metal.
Exercises
added
A carbon steel hollow bush has finished machined dimensions: outside diameter = 120 mm, bore diameter = 50 mm, and length = 80 mm. Allowing 3.0 mm machining allowance per surface and 20 mm/m (2%) shrinkage allowance for carbon steel, calculate the required pattern outside diameter, core-box bore diameter, and pattern length.
Compute rough cast dimensions (with 3.0 mm machining allowance per surface):
- Rough OD = 120 + (2 x 3.0) = 126.0 mm
- Rough Bore ID = 50 - (2 x 3.0) = 44.0 mm
- Rough Length = 80 + (2 x 3.0) = 86.0 mm
Apply 2% carbon steel shrinkage allowance (factor = 1.02):
- Pattern OD = 126.0 x 1.02 = 128.52 mm
- Core-box Bore ID = 44.0 x 1.02 = 44.88 mm
- Pattern Length = 86.0 x 1.02 = 87.72 mm
Pattern OD = 128.52 mm, core-box bore ID = 44.88 mm, pattern length = 87.72 mm.
Apply forging volume conservation (neglecting scale loss) to find: (a) The final length when a 24 mm diameter, 150 mm long mild steel rod is drawn down uniformly to 16 mm diameter. (b) The final length when a 25 mm x 25 mm square bar of 80 mm heated length is upset uniformly to a 35 mm x 35 mm square section.
(a) Drawing down 24 mm bar to 16 mm:
- L2 = L1 x (d1 / d2)^2 = 150 x (24 / 16)^2 = 150 x (1.5)^2 = 150 x 2.25 = 337.5 mm.
(b) Upsetting 25 mm square bar to 35 mm square:
- L2 = (A1 x L1) / A2 = (25 x 25 x 80) / (35 x 35) = 50000 / 1225 = 40.82 mm.
(a) Drawn-down length = 337.5 mm; (b) Upset length = 40.82 mm.
Name the main parts of a blacksmith's anvil and state the function of fullers, swages, flatter, and hardie. Also distinguish between upsetting and drawing down in forging.
Anvil parts and shaping tools:
- Anvil parts: Flat hardened face (hammering surface), tapered horn/beak (bending rings/curves), step (soft cutting ledge), square hardy hole (holds shanks of hardie/bottom swages), and round pritchel hole (clearing punched slugs).
- Fullers (top & bottom): Rounded-edge tools used in pairs to groove and draw out stock rapidly.
- Swages (top & bottom): Semicircular grooved dies used to finish round, hex, or square bars smoothly.
- Flatter: Broad flat-faced block struck with a sledgehammer to remove hammer dents and level flat faces.
- Hardie: Wedge-shaped chisel fitting upright in the hardy hole to cut hot bars from underneath.
Upsetting vs. Drawing down:
- Upsetting (jumping): Compressing a heated bar axially along its length to increase cross-sectional area and decrease length (e.g., forming bolt heads).
- Drawing down: Hammering a heated bar transversely (using cross-peen or fullers) to increase length and decrease cross-sectional thickness.
Anvil has face, horn, step, hardy hole, and pritchel hole. Fullers groove/draw out, swages size round/hex bars, flatter smooths flat faces, hardie cuts hot stock. Upsetting thickens & shortens; drawing down thins & lengthens.
Explain the four primary pattern allowances used in sand casting, clearly stating why each allowance is necessary and whether it increases or decreases pattern dimensions.
Explain the four primary pattern allowances:
- Shrinkage (Contraction) Allowance: Compensates for solid thermal contraction of the casting cooling from freezing temperature to room temperature (e.g., 10 mm/m for grey cast iron, 20 mm/m for steel). Applied positively using a shrink rule.
- Draft (Taper) Allowance: Slight 1–3 degree taper on vertical faces parallel to pattern withdrawal so the pattern lifts cleanly without crumbling sand walls (usually added positively to external surfaces).
- Machining (Finishing) Allowance: Extra 1.5–5 mm metal added to faces requiring subsequent lathe/mill finishing so surface scale/roughness can be machined off (+ on external faces, - on internal bore diameters).
- Distortion (Camber) & Shake Allowances: Pre-bending U/T-shaped patterns in the opposite direction to offset cooling warpage; shake allowance is a small negative correction compensating for pattern rapping enlargement.
- Shrinkage (counters thermal contraction on cooling; + via shrink rule); 2. Draft (1–3 deg vertical taper for clean withdrawal); 3. Machining (1.5–5 mm extra stock on machined faces; + OD, - ID); 4. Distortion/Shake (counters uneven cooling warpage / rapping enlargement).
What is a core in foundry practice and how are core prints used to support it? State the main ingredients of green moulding sand and explain the purpose of sprue, riser, and vent holes in a sand mould.
Cores, core prints, and green moulding sand:
- Core & Core Prints: A core is a pre-baked, permeable sand insert placed inside the mould cavity to form internal holes, cavities, or passages. Core prints are projections added to the pattern that mould matching pockets in the sand to support and locate the core securely against molten metal lift.
- Green Sand Ingredients: Silica sand (75–85%, refractory base) + clay/bentonite (8–15%, binder) + water (4–6%, activates clay) + additives like sea-coal dust (improves finish).
Roles of sprue, riser, and vent holes:
- Sprue: Vertical tapered passage cut in the cope leading molten metal from the pouring basin into the runner/ingates and cavity.
- Riser: Vertical reservoir connected to the thickest casting section; feeds liquid metal to compensate for liquid-to-solid shrinkage and shows when the mould is completely filled.
- Vent Holes: Fine pinholes pricked through the sand with a vent wire so steam and hot mould gases escape freely instead of trapping inside as blowholes.
A core forms internal holes/passages and rests in pockets formed by core prints. Green sand = silica sand + bentonite clay + water (+ coal dust). Sprue feeds molten metal down into gates; riser feeds liquid shrinkage and confirms mould fill; vent holes let steam/gases escape to prevent blowholes.