Welding
Open in the Padhaiko app7.1 Arc welding
Welding is a permanent joining process in which two or more metal pieces are coalesced by heating them to a molten or plastic state, with or without pressure and with or without filler metal. Electric Arc Welding (commonly Manual Metal Arc Welding / SMAW) uses the intense heat of a sustained electric arc (~3500–4000 deg C) struck between a consumable electrode and the workpiece to melt both the base metal edges and the electrode tip into a unified weld pool.
Arc Welding Equipment and Accessories
| Item | Function & Technical Notes |
|---|---|
| Power Source (AC / DC) | Steps down mains voltage (220/415 V) to safe open-circuit striking voltage (50–90 V) and high welding current (50–400 A); AC transformer (low cost, minimal arc blow) or DC rectifier/inverter (smooth arc, selectable polarity: DCEP for deep penetration, DCEN for thin sheets/fast melt) |
| Electrode Holder | Insulated spring-jaw clamp gripping the bare stub end of the coated electrode cleanly |
| Work (Earth) Clamp | Heavy copper/brass clamp securing the return lead directly onto the clean workpiece or steel welding table |
| Welding Cables | Flexible multi-strand insulated copper cables carrying current from machine to holder and back from work clamp |
| Welding Helmet / Hand Shield | Protects face and eyes from intense UV/IR arc radiation and hot spatter; fitted with dark filter glass (Shade 10–12) behind a replaceable clear cover glass |
| Chipping Hammer & Wire Brush | Pointed/chisel hammer knocks off brittle solidified slag after the weld cools; stiff wire brush cleans rust before welding and slag residue between multi-pass beads |
| Protective Apparel | Heavy leather apron, leather gauntlet gloves, leather sleeves/leggings, and high-top safety boots |
Influencing Factors in Arc Welding
Weld bead appearance, penetration depth, and structural soundness depend on five controllable variables:
- Welding Current (Amperage): Governs melt rate and penetration. Practical workshop guide: 30 to 40 A per mm of electrode core diameter (for example, 100–125 A for a 3.15 mm electrode). Too low causes sticking, poor fusion, and trapped slag; too high causes excessive spatter, undercut along bead edges, and burn-through.
- Arc Length: Distance from molten electrode tip to molten weld pool—ideally kept roughly equal to the electrode core diameter (2–4 mm). Too long makes the arc wander, increases spatter, and lets air oxidize the molten metal (porosity/brittleness); too short freezes the electrode onto the plate.
- Travel Speed: Rate of moving along the joint. Too slow piles up a wide, humped bead and overheats thin plates; too fast produces a narrow, ropy bead with incomplete fusion.
- Electrode Angles: Inclined 70–80 degrees along the direction of travel (drag/travel angle) and centered (45 deg for fillet welds, 90 deg for flat butts) across the joint.
- Polarity & Arc Blow: DC permits DCEP (electrode positive — 2/3 heat at workpiece, deeper penetration) or DCEN (electrode negative — faster rod burn-off for thin sheet); AC eliminates magnetic arc blow at corners and edges.
Methods of Striking an Arc (Tap and Scratch)
| Aspect | Scratch Method | Tap (Touch-and-Lift) Method |
|---|---|---|
| Technique | Drag the electrode tip lightly across the plate like striking a match, then lift 2–4 mm immediately as sparks appear | Lower the electrode vertically to lightly tap the plate, then snap upward immediately by 2–4 mm |
| Difficulty | Easier for beginners; less likely to freeze/stick to the base metal | Requires steadier wrist control to avoid sticking |
| Surface Mark | Leaves light scratch/arc strikes if performed outside the weld groove | Minimal surface marring; ideal inside narrow V-grooves and finished jobs |
(If an electrode sticks firmly, twist/snap the holder sideways immediately or release the holder jaws—never stare at the glowing rod without a shield while freeing it.)
Electrodes and Flux Coating Functions
An arc welding electrode consists of a solid metal core wire (diameter 2.0, 2.5, 3.15, 4.0, 5.0 mm; length 350–450 mm) wrapped in an extruded flux coating (rutile, cellulosic, or basic/low-hydrogen):
- Shielding Gas Cloud: Decomposes in the arc to surround molten droplets with CO2/CO, keeping atmospheric oxygen and nitrogen out.
- Protective Slag Blanket: Floats over the hot weld bead, slowing cooling rate and shielding it from oxidation.
- Arc Stabilization: Contains potassium/sodium compounds that ionize easily so the arc reignites smoothly on AC cycles.
- Deoxidizing & Alloying: Cleans impurities and adds alloying elements (Mn, Si) to match base metal strength.
Types of Weld Joints and Welding Positions
- Five Basic Weld Joints:
- Butt Joint: Edges meet end-to-end in the same plane (square groove for thin plates <= 5 mm; single-V or double-V bevelled grooves for thicker plates).
- Lap Joint: One plate overlaps the other; joined with fillet welds along edges.
- Tee (T) Joint: Two plates meet at 90 degrees forming a T; joined by fillet welds.
- Corner Joint: Two plates meet at an L-corner (flush, half-open, or full-open).
- Edge Joint: Parallel edges of two thin sheets welded along their common rim.
- Four Standard Welding Positions:
- Flat (Downhand — 1G / 1F): Work lies horizontal beneath the electrode; fastest, easiest, highest quality.
- Horizontal (2G / 2F): Weld axis is horizontal on a vertical wall; molten metal tends to sag downward.
- Vertical (3G / 3F): Weld progresses vertically upward (deep penetration) or downward (thin sheet speed).
- Overhead (4G / 4F): Welding from underneath; hardest position requiring lower current, short arc, and fast freeze electrodes.
TIG (GTAW) and MIG (GMAW) Welding
| Aspect | TIG Welding (GTAW) | MIG Welding (GMAW) |
|---|---|---|
| Electrode Type | Non-consumable thoriated/ceriated tungsten electrode | Continuously fed consumable solid wire spool |
| Filler Metal | Added separately by hand with a bare filler rod (or autogenous with no filler) | The consumable wire electrode itself melts as filler metal |
| Shielding Gas | Pure Argon or Helium (inert gases) | Argon, CO2 (MAG for steel), or Ar + CO2 mixture |
| Control & Speed | Slow, two-handed precision process (foot pedal/torch + filler rod) | Fast, semi-automatic one-handed gun trigger; high deposition rate |
| Best Applications | Thin stainless steel, aluminium, magnesium, titanium, precision aerospace/pipe root passes | Structural steel, automotive frames, thick aluminium fabrication, production lines |
7.2 Gas welding: Oxyacetylene gas welding, oxyacetylene gas welding accessories, filler rods, fluxes, types of flames and uses
Oxyacetylene Gas Welding (OAW) melts base metal edges and a filler rod using the high-temperature chemical flame (~3100–3300 deg C) produced by burning acetylene (C2H2) with pure oxygen (O2) inside a hand-held welding torch.
- Two-Stage Combustion:
- Primary combustion (inner cone): C2H2 + O2 -> 2CO + H2 + Heat (oxygen comes from the cylinder).
- Secondary combustion (outer envelope): Carbon monoxide and hydrogen burn with atmospheric oxygen to form CO2 and H2O vapor, shielding the weld pool from ambient air.
- Welding Techniques: Leftward (forehand) welding points the torch forward into the unwelded seam ahead of the rod (good for thin sheets <= 5 mm); Rightward (backhand) points the torch back at the completed bead ahead of the rod (faster and deeper penetration for plates > 5 mm).
Oxyacetylene Gas Welding Accessories
| Component | Key Identification & Safety Features |
|---|---|
| Oxygen Cylinder | High-pressure seamless steel cylinder painted black (or dark green), charged up to 140–150 bar; brass valve has Right-Hand (RH) threads |
| Acetylene Cylinder | Short, wide cylinder painted maroon, packed with porous calcium-silicate mass soaked in acetone (dissolves C2H2 safely below ~15–17 bar—free C2H2 explodes above 2 bar!); valve has Left-Hand (LH) threads |
| Pressure Regulators | Reduce high cylinder pressure down to safe working torch pressure (0.15–1.0 bar for C2H2; 0.5–3.0 bar for O2); dual gauges show bottle pressure and hose line pressure |
| Hoses & Nut Coding | Twin rubber hoses: Blue/Black/Green for Oxygen (RH brass union nuts); Red/Maroon for Acetylene (LH brass union nuts with notched hex corners so hoses can never be swapped) |
| Flashback Arrestors | Non-return check valves + sintered flame traps fitted at torch/regulators to stop flame traveling back into cylinders |
| Welding Torch (Blowpipe) | Brass body with Oxygen and Acetylene needle valves, internal mixing chamber, and interchangeable copper nozzle tips sized by plate thickness |
| Spark Lighter & Goggles | Friction flint spark lighter (never use matches or cigarette lighters!); green/dark gas-welding goggles (Shade 4–6) |
Filler Rods and Fluxes
- Filler Rods: Uncoated metal rods (typically 900 mm long, 1.6 to 6 mm diameter) matching or slightly exceeding base metal strength—copper-coated mild steel rods for MS, silicon-cast-iron rods for grey cast iron, and aluminium/brass alloys for non-ferrous jobs.
- Fluxes: Chemical cleaning compounds (powders or pastes of borax, boric acid, alkali chlorides/fluorides) applied to the joint and hot filler rod tip to dissolve stubborn surface oxides (such as Al2O3 on aluminium or Cr2O3 on stainless steel) and improve molten metal wetting. Note: Clean mild steel normally welds without flux in oxyacetylene welding, whereas cast iron, brass, bronze, copper, stainless steel, and aluminium require flux.
Types of Oxyacetylene Flames and Uses
Adjusting the oxygen-to-acetylene valve ratio yields three distinct flame types:
| Flame Type | O2 : C2H2 Ratio | Visual Appearance & Inner Cone Temp | Metals Welded & Specific Uses |
|---|---|---|---|
| 1. Neutral Flame | Balanced (~1 : 1 to 1.1 : 1) | Two zones: crisp, rounded luminous white inner cone + light blue outer envelope; quiet steady burn (~3200 deg C) | Mild steel, stainless steel, cast iron, copper, aluminium (does not oxidize or add carbon) |
| 2. Carburizing (Reducing) Flame | Excess Acetylene (ratio < 1, e.g. 0.85 : 1) | Three zones: bright inner cone + ragged whitish acetylene feather + blue outer envelope (~2900–3000 deg C) | High-carbon steels, alloy steels, hard-facing (Stellite), nickel/Monel, brazing/silver soldering, aluminium (mildly reducing) |
| 3. Oxidizing Flame | Excess Oxygen (ratio > 1, e.g. 1.2–1.5 : 1) | Two zones: short, sharply pointed inner cone + narrow purplish envelope + loud roaring hiss (~3300–3400 deg C) | Brass and bronze (excess oxygen forms a thin protective zinc-oxide film that stops toxic zinc fuming); unsuitable for steel (causes foamy brittle welds) |
Worked Examples
1
During manual shielded metal arc welding (SMAW) on mild steel using a 3.15 mm coated electrode: (a) Estimate a suitable starting welding current using the workshop 30–40 A/mm rule (take 35 A/mm). (b) If the arc runs at V = 24 V and I = 120 A with an arc thermal efficiency eta = 0.80 and travel speed v = 180 mm/min, calculate the total arc power (W) and the net heat input per millimetre of weld (J/mm).
(a) Estimate starting welding current:
- Electrode core diameter d = 3.15 mm.
- Using 35 A/mm rule: I_est = 35 x 3.15 = 110.25 A (within the standard 95–125 A range for 3.15 mm rutile electrodes).
(b) Calculate arc power and net heat input per mm:
- Total electrical arc power: P = V x I = 24 x 120 = 2880 W (2.88 kW).
- Net heat input per mm: H_net = (0.80 x 24 x 120 x 60) / 180 = 138240 / 180 = 768.0 J/mm (0.768 kJ/mm).
(a) Starting current ~ 110 A (95–125 A range); (b) Total arc power = 2880 W, net heat input = 768.0 J/mm.
2
An oxyacetylene welding nozzle consumes 450 litres/hour of acetylene gas. (a) How many litres/hour of oxygen are drawn from the cylinder for (i) a neutral flame (O2:C2H2 = 1.0:1) and (ii) an oxidizing flame (O2:C2H2 = 1.3:1)? How much extra oxygen per hour does the oxidizing flame use? (b) If the acetylene cylinder holds 2700 litres of usable gas, how many hours of continuous welding can it supply at 450 L/hr?
(a) Oxygen consumption for neutral vs. oxidizing flames:
- Neutral flame (1.0 : 1): Oxygen flow = 450 x 1.0 = 450 L/hr.
- Oxidizing flame (1.3 : 1): Oxygen flow = 450 x 1.3 = 585 L/hr.
- Extra oxygen required per hour = 585 - 450 = 135 L/hr.
(b) Continuous welding duration from acetylene cylinder:
- Operating duration = Usable gas volume / Consumption rate = 2700 / 450 = 6.0 hours.
(a) Neutral flame draws 450 L/hr O2; oxidizing flame draws 585 L/hr O2 (135 L/hr extra); (b) Cylinder supplies 6.0 hours of welding.
3
Write the exact safe ignition, neutral-flame adjustment, and shut-down sequence for an oxyacetylene gas welding torch, explaining why the shut-down valve order differs from the lighting order.
Pre-check, lighting, and adjusting to a Neutral flame:
- Stand to the side of regulators (never in front of gauge glass), crack and close cylinder valves briefly to blow dust out before attaching regulators, then open cylinder valves slowly (acetylene valve only 1/2 to 1 turn so it can be shut instantly in an emergency).
- Set working pressures on both regulators (typically ~0.3–0.5 bar acetylene, ~1.0–1.5 bar oxygen).
- Open the torch Acetylene valve ~1/4–1/2 turn and ignite immediately with a flint spark lighter (never a match). Adjust acetylene until soot/black smoke stops and the flame sits steadily against the nozzle tip.
- Slowly open the torch Oxygen valve: the yellow smoky flame turns into a three-zone carburizing flame (with an acetylene feather). Continue opening oxygen gently until the feather pulls back and merges completely into a crisp, rounded white inner cone—this is the Neutral Flame.
Safe shut-down sequence (critical valve order):
- Close the torch Acetylene valve first (flame goes out cleanly), then close the torch Oxygen valve.
- Close both main cylinder valves tightly.
- Re-open torch valves one at a time to bleed pressure gauges to zero, close torch valves gently, and back out both regulator T-screws until loose.
Light: Open acetylene slightly -> ignite with flint spark lighter -> slowly open oxygen until the feather disappears into a crisp rounded inner cone (Neutral flame). Shut down: Close torch acetylene valve first, then torch oxygen valve, close cylinders, and bleed hoses/regulators to zero.
Exercises
added
(a) Estimate a suitable welding current for a 4.0 mm mild steel electrode using the 35 A/mm workshop guideline. (b) An arc welder operates at 26 V and 150 A with thermal efficiency eta = 0.75 and travel speed 150 mm/min. Calculate the arc power (W) and net heat input per millimetre of weld (J/mm).
(a) Estimate current for 4.0 mm electrode:
- I_est = 35 x 4.0 = 140 A (typical range 130–170 A).
(b) Calculate arc power and net heat input per mm:
- Total arc power: P = V x I = 26 x 150 = 3900 W (3.90 kW).
- Net heat input per mm: H_net = (eta x V x I x 60) / v = (0.75 x 26 x 150 x 60) / 150 = 175500 / 150 = 1170.0 J/mm.
(a) Estimated current = 140 A; (b) Arc power = 3900 W, net heat input = 1170.0 J/mm.
An oxyacetylene torch welding brass uses an oxidizing flame (O2 : C2H2 ratio = 1.4 : 1) with an acetylene consumption rate of 360 litres/hour. Calculate the oxygen consumption rate (L/hr) and determine how long a 3600-litre usable oxygen cylinder will last at this setting.
Compute oxygen consumption rate:
- Oxygen flow rate = 1.4 x Acetylene flow rate = 1.4 x 360 = 504 L/hr.
Compute oxygen cylinder operating duration:
- Duration = Usable O2 volume / O2 flow rate = 3600 / 504 = 7.14 hours (approx. 7 hours 9 minutes).
Oxygen consumption rate = 504 L/hr; a 3600 L oxygen cylinder lasts 7.14 hours (approx. 7 h 9 min).
Explain the tap and scratch methods of striking an electric arc, list four functions of the flux coating on an arc welding electrode, and describe the defects caused by excessive arc length and excessive current.
Arc striking methods and flux coating functions:
- Scratch method: Brush the electrode lightly across the plate like a match and lift 2–4 mm as the arc ignites (easier for beginners, leaves light surface marks).
- Tap method: Touch the tip vertically to the work and snap upward 2–4 mm immediately (cleaner inside narrow grooves, needs steady wrist control).
- Four functions of flux coating: (1) Produces shielding gas to exclude O2/N2; (2) Forms a protective slag blanket slowing cooling; (3) Stabilizes the arc via easily ionized salts; (4) Deoxidizes and adds alloying elements to the weld metal.
Defects from excessive arc length and excessive current:
- Excessive arc length (> electrode diameter): Causes unstable wandering arc, heavy spatter, poor penetration, and air contamination leading to gas porosity and brittle welds.
- Excessive welding current: Causes deep undercut along the bead toes, excessive spatter, overheating distortion, and burn-through on thin plates.
Scratch drags & lifts 2–4 mm; Tap touches vertically & lifts 2–4 mm. Flux coating provides shielding gas, slag protection, arc stability, and deoxidation/alloying. Long arcs cause spatter, poor penetration, and porosity; excessive current causes undercut, spatter, and burn-through.
Compare TIG (GTAW) and MIG (GMAW) welding processes across electrode type, shielding gas, filler feeding, and primary applications. Also name the five basic weld joints and four standard welding positions.
Compare TIG vs. MIG welding:
- TIG (GTAW): Uses a non-consumable tungsten electrode, pure Argon or Helium inert gas, and a separate hand-fed filler rod. Slower, cleaner, ultra-precise; ideal for thin stainless steel, aluminium, magnesium, and critical pipe root welds.
- MIG (GMAW): Uses a continuously fed consumable wire spool, shielding gas (Argon, CO2, or Ar+CO2), and automatic wire feed through a trigger gun. Much faster deposition rate; ideal for structural steel, automotive, and production fabrication.
Five weld joints and four welding positions:
- Five joints: Butt, Lap, Tee (T), Corner, and Edge joints.
- Four positions: Flat (downhand), Horizontal, Vertical, and Overhead.
TIG (non-consumable tungsten + Ar/He + manual rod, slow precision on thin Al/SS) vs. MIG (consumable wire spool + Ar/CO2 + semi-automatic gun, fast production). Joints: Butt, Lap, Tee, Corner, Edge. Positions: Flat, Horizontal, Vertical, Overhead.
Sketch/describe in words the three types of oxyacetylene flames (Neutral, Carburizing, and Oxidizing), stating their O2 : C2H2 ratio, flame zones, approximate inner-cone temperature, and applications. Also explain why acetylene cylinders contain acetone and use left-hand notched threads.
Compare the three oxyacetylene flames:
- Neutral Flame (O2:C2H2 ~ 1:1): Crisp rounded white inner cone (~3200 deg C) + pale blue outer envelope; quiet burn. Used for mild steel, stainless steel, cast iron, copper, and aluminium.
- Carburizing Flame (O2:C2H2 < 1, excess C2H2): Three zones—inner cone + luminous white acetylene feather + outer envelope (~2900–3000 deg C). Used for high-carbon steel, hard-facing, alloy steels, and nickel alloys.
- Oxidizing Flame (O2:C2H2 > 1, excess O2): Short, sharp pointed inner cone + purplish envelope + loud hissing sound (~3300–3400 deg C). Used for brass and bronze (forms protective oxide skin preventing zinc evaporation); unsuitable for steel.
Acetylene cylinder safety design:
- Pure acetylene becomes explosively unstable above ~2 bar pressure; storing it dissolved in acetone absorbed in a porous filler inside the maroon cylinder allows safe storage up to ~15–17 bar.
- Acetylene fittings use left-hand (LH) threads with notched hex nuts (while oxygen uses standard RH un-notched threads) so fuel and oxygen hoses/regulators can never be accidentally interchanged.
Neutral (1:1, 2 zones, ~3200 C — steel/cast iron/Cu/Al); Carburizing (<1, 3 zones with feather, ~2950 C — high-C steel/hard-facing); Oxidizing (>1, pointed cone & hiss, ~3350 C — brass/bronze). Acetylene is dissolved in acetone inside a porous mass to prevent explosion above 2 bar, and uses LH notched threads to prevent hose mix-ups with RH oxygen lines.